How to read an ISO 12944-6 test report before choosing a coating
When a manufacturer says its paint "complies with ISO 12944", the only thing that proves it is the test report. But a report has many pages and tables. These are the points to look at to know whether it backs up what is claimed.
1. Exactly which category was tested?
ISO 12944-6 doesn't give a general pass: each test corresponds to a combination of corrosivity (C2, C3, C4, C5) and durability (low, medium, high or very high). A report for C3 medium is no use for a C5 project. Look in the scope of the test for the specific category, for example "C4 very high and C5 high".
2. How many hours did each test last?
The more demanding the category, the more hours the standard requires. For example, for C4 very high and C5 high it requires 1,440 hours of salt spray (ISO 9227) and 720 hours of condensation (ISO 6270-1). Check that the hours in the report match the category being claimed.
3. At what thickness was it tested?
It's the most overlooked figure and the most important. A good report measures the dry film thickness of each panel (ISO 2808). If the test was passed with 160 µm, you can't expect the same result applying 60 µm. The thickness on your project must be at least that of the test.
4. How are the appearance results read?
After ageing, the coating is assessed according to ISO 4628:
Blistering (ISO 4628-2): expressed as quantity and size, for example 0(S0) if there is none.
Rusting (ISO 4628-3): from Ri 0 (no rust) to Ri 5 (40-50% of the surface rusted).
Cracking (ISO 4628-4) and flaking (ISO 4628-5): from 0 (none) to 5.
To pass, ISO 12944-6 requires the best rating in all of them: no blistering, no rust, no cracking and no flaking.
5. How far did corrosion creep from the scribe?
Before the salt spray, the coating is scratched down to the steel. At the end, the corrosion creep from that scribe is measured; the standard allows a maximum of 1.5 mm. This figure says a lot about how the coating will behave when it takes a knock on site. With a well-formulated zinc-rich coating, creep can be 0 mm.
6. Was adhesion maintained?
The cross-cut test (ISO 2409) is done at the start and after each ageing. The scale goes from 0 (perfect) to 5. ISO 12944-6 allows 0 to 2. Make sure it was also measured after the tests, not just at the start.
7. Who did it, and on which product?
Check that the laboratory is independent, that the report is signed and dated, and that the sample corresponds to the product you are going to buy. Also look at the notes: some laboratories state which tests are within their accreditation and which are not.
Warning signs
The manufacturer provides a one-page "certificate" without result tables.
The report doesn't state the thickness of the panels.
The tested category is lower than the one being claimed.
There is only salt spray, with no humidity test, or vice versa.
Adhesion was only measured at the start.
How we apply it at GALVANOL
GALVANOL was tested according to ISO 12944-6:2018 for C4 very high and C5 high in an independent laboratory: 1,440 hours of salt spray and 720 hours of humidity, with average thicknesses of 130 to 163 µm, no blistering, no rust, 0 mm creep from the scribe and adhesion within requirements. We explain it in detail in our article about the test.
Do you have a project in a C4 or C5 environment? We are the manufacturer: write to info@galvanol.eu and we'll help you define the thickness and system. Technical and safety data sheets are in Products.



Comments