How to protect cuts, drill holes and scuffs on solar park structures

GALVANOL IBERIA SL
1 hour ago
3 min read

Solar park structures arrive galvanized from the factory, but assembly leaves its mark: cuts to size, new drill holes, scuffs when fitting profiles, damaged bolts or site welds. At each of those points the steel is left bare and, within a few months, rust appears. Repairing them properly during construction costs little; doing it once the plant is producing costs much more.

Where corrosion appears in a solar park

  • Cuts and drill holes made on site: the cut edge has no zinc.

  • Scuffs and knocks during transport, unloading and assembly.

  • Bolted joints: washers and bolts damaged when tightening.

  • Welds on piles, frames or supports: the heat burns off the galvanizing.

  • The base of driven posts, where friction with the ground strips off coating.

The environment decides: ISO 12944 corrosivity categories

ISO 12944-2 classifies environments by how aggressive they are. A park in a dry rural area is usually C2 or C3; near the coast, industrial areas or with high humidity, it can reach C4 or C5. The more aggressive the environment, the more important it is to repair in time and with the right thickness.

According to the tests in the GALVANOL technical data sheet (ISO 12944-6), a coating of 80 µm or more in 1-2 coats gives an estimated durability of more than 25 years in C3, 15 to 25 years in C4 and 7 to 15 years in C5.

On-site touch-up protocol

  1. Inspect and mark. Walk the rows after assembly and mark unprotected cuts, drill holes, scuffs and welds.

  2. Clean. Remove rust, burrs and slag with a brush or flap disc (180-220 grit) and degrease. Also prepare a small margin of sound galvanizing around it.

  3. Apply the same day. Don't let more than 12 hours pass between cleaning and application outdoors.

  4. Use the spray for spot touch-ups. Shake GALVANOL Spray well (the ball should rattle freely) and apply at 25-35 cm in thin coats. For large surfaces or welds, a brush with GALVANOL from the can is better.

  5. Reach the thickness. Apply coats until you exceed the thickness required by the project specification; if working to ISO 1461, the repair must reach at least 100 µm unless otherwise agreed.

  6. Record. Measure the dry film thickness on a sample of repairs and keep it in the project's quality dossier.

How much product do you need?

As a guide, a 500 ml GALVANOL spray covers about 1.5 m² per coat at 40-60 µm. To calculate buckets and cans for your surface and thickness, use the calculator on the Products page.

Why cold galvanizing and not a silver paint

Silver aluminium paints or low-zinc primers look like galvanizing, but they don't protect the same way. GALVANOL contains a minimum of 96% zinc in the dry film and provides cathodic protection: the zinc sacrifices itself before the steel, just as in hot-dip galvanizing. That's why it is suitable for repairing galvanizing according to ISO 1461 and ASTM A780. If you also want a bright metallic finish, you can apply ALINOL Spray over GALVANOL, never instead of it.

Other points to watch

  • Piles and structure feet: the area in contact with the ground is the first to lose zinc.

  • Cable boxes, trays and supports exposed to the weather.

  • Floating or coastal plants: they need more thickness (C4–C5).

  • Older plants: top up the zinc before red rust appears (how to do it).

Tip for installers: keep a GALVANOL Spray in every van and touch up each cut on the spot. A few seconds of touch-up prevents a claim years later.

Do you build or maintain solar parks? We'll send you technical data sheets and project terms and help you calculate quantities. Write to us at info@galvanol.eu or visit our page on photovoltaics.

General guide. For each project, the structure manufacturer's technical specification and the requirements agreed with the owner take precedence.

 
 
 