How to prepare the surface before applying cold galvanizing
Cold galvanizing only protects if the zinc is in direct contact with the steel. If rust, grease, old paint or dust remains between the two, cathodic protection doesn't work and the coating can peel off. That is why surface preparation is the most important part of the job.
The goal: clean, dry, rough steel
Cleanliness: grade Sa 2½ according to ISO 8501-1 where blasting is possible.
Roughness: the GALVANOL data sheet recommends an Rz profile of 50-70 µm (Ra 12.5 µm), which improves anchoring.
No grease or salts: always degrease after cleaning.
Depending on the condition of the steel
New steel
Blast to Sa 2½ and degrease. New rolled steel has mill scale, which must be removed: cleaning it is not enough.
Rusty steel or old galvanizing
Remove rust and contamination by hand or mechanical means, with high-pressure water (10-20 MPa) or Sa 2½ blasting, and degrease. On small areas you can use sandpaper or a 180-220 grit flap disc.
Painted steel
The paint must be removed: cold galvanizing cannot protect through a layer of paint. This can be done with chemical stripper, ultra-high-pressure water (175-275 MPa) or Sa 2½ blasting, followed by degreasing.
Damaged hot-dip galvanizing
Clean the damaged area down to sound steel or zinc, remove rust and degrease, including a margin around it so the repair overlaps onto the existing galvanizing.
Times and conditions
Apply no later than 12 hours after preparation if the part is outdoors, and 48 hours if it is indoors.
Maximum relative humidity 90%. The surface must be dry, with no condensation.
GALVANOL in cans can be applied between -30 °C and +60 °C; the spray between +5 °C and +40 °C.
Common mistakes
Applying over rust "because the zinc converts it": it is not a rust converter.
Degreasing before sanding instead of after: dust and grease come back to the surface.
Letting days pass between preparation and application.
Aged galvanizing
If the galvanizing is old but still intact, clean off the white zinc salts, degrease and apply directly to recharge the protection. We explain it in how to recharge old galvanizing.
Recommended tools
Steel wire brush, scraper or disc for rust, 180–220 grit sandpaper or flap disc, and a cloth with xylene for degreasing.
If you have doubts about how to prepare a specific surface, write to us at info@galvanol.eu. The full technical data sheets are in Products.



Comments