Corrosion on catenary masts and portals: where it starts and how to repair it
Updated: 3 hours ago
A galvanized catenary mast can last for decades. But it does not rust all at once or evenly: corrosion starts at a few specific points and, if nobody stops it, spreads from there. Knowing where to look is half the job.
The five points where corrosion starts
The base of the mast: the joint with the concrete foundation or anchor plate collects water, mud, leaves and salts. It is the hardest-hit point and the one that most affects the stability of the mast.
Anchor plates and bolts: on viaducts, masts are anchored with steel elements and bolts; nuts tightened after galvanizing and covered areas trap moisture.
Installation drill holes and cuts: every hole drilled on site to fix cantilevers, stays or supports leaves bare steel at the edge.
Site welds: the heat burns off the zinc around the bead, and slag stops any coating from adhering if it is not cleaned off.
Cantilevers, stays and fittings: small, highly exposed parts that are handled every time the catenary is adjusted.
How to recognize each stage
White rust: whitish powder on the zinc. Normal in small amounts, but if it is heavy it means the zinc is being consumed quickly.
Brown stains: the zinc layer is already very thin. This is the ideal moment to act.
Red rust: the steel is under attack. Repair as soon as possible to stop loss of section.
The environment changes everything
The speed of corrosion depends on the environment. ISO 12944 classifies it from C1 (very low) to CX (extreme). A dry inland section may be C2 or C3, while catenary near the sea, next to industrial estates or on mountain passes with de-icing salts can be C4 or C5. On those sections the zinc is consumed much faster and inspections should be more frequent.
Step-by-step repair on site
Prepare: remove rust, mill scale, slag and dirt down to clean metal with a wire brush, disc or Sa 2½ blasting, and degrease.
Stir GALVANOL well: zinc is heavy and settles at the bottom.
Apply by brush, roller, spray gun or spray can: thin coats, the first of about 60 µm (2.4 mils) and the following ones of 60–80 µm (3.1 mils), overlapping a few centimetres onto the sound galvanizing.
Reach the thickness: minimum 105 µm (4.1 mils) dry on structural elements such as masts and portals (about 490 g/m²) and 69 µm (2.7 mils) on non-structural parts.
Check: measure with a thickness gauge and allow the full 72-hour cure before applying topcoats.
Why GALVANOL
GALVANOL is a cold galvanizing with a minimum of 96% zinc in the dry film (ISO 3549) that complies as a galvanizing repair to ISO 1461 and ASTM A780. In tests to ISO 12944-6 at an accredited laboratory it achieved a C4 very high and C5 high classification, with 0 mm corrosion creep from the scribe. It is applied from −30 °C to +60 °C and is touch-dry in about 20 minutes, so it fits short maintenance windows. For the shine of new galvanizing, it can be finished with ALINOL Spray.
Read on: GALVANOL for railways and Preventive maintenance of railway steel.